Anders Rand Andersen
Søren Rodahl Thisted
Degradation of the conductive path in photovoltaic (PV) strings is a frequent cause of energy loss and, in some cases, of safety incidents. It manifests as an increase in the series resistance of the string. In SOLARIS, emazys investigates how series resistance can be measured with impedance methods, and how such measurements can be automated and performed repeatedly on installed strings.
About SOLARIS
The objective of SOLARIS is to develop and demonstrate physical and digital tools for more efficient and reliable operation and maintenance (O&M) of PV plants. These include weather and power forecasting, novel wind, dust and impedance sensors, multispectral drone inspection, early fault detection, reconfigurable power electronics and an IoT platform that feeds a PV asset management software. The project targets a performance index of 90%, an availability above 98% and a 10% reduction in the levelised cost of energy. The tools will be demonstrated in eight use cases across Europe, covering utility-scale and small-scale ground-mounted, rooftop, floating and agrivoltaic systems. emazys contributes the impedance sensing technology.
Series resistance in PV strings
Every conductive path through which current flows, including metal contacts, semiconductor layers, ribbons, cables, and connectors, offers some resistance to current flow. The cumulative resistance along the current path constitutes the total series resistance, which produces a voltage drop and associated power loss that increase with current.
At cell level, the series resistance is the sum of the ohmic contributions of the cell structure: [1, 2]:
Rs,cell = Rbb + Rf + Rfc + Re + Rb + Rbc (1)
In a module, the cells are connected in series by interconnect ribbons, and groups of cells are protected by bypass diodes. At string level, the measured series resistance therefore also includes the contributions outside the cells:
Rs,string = Σ (Nc Rs,cell + Rint) + Rjb + Rcable + Rconn (2)
where Nc is the number of cells per module, Rint the resistance of the cell interconnects and solder joints in each module, Rjb the junction box contributions, Rcable the module and string cable resistance and Rconn the sum of the connector contact resistances. In a new installation this value is low and stable, and the contributions in (2) that are most exposed to ageing are the solder joints, interconnects and connectors.
During operation, several mechanisms increase the series resistance. Connectors may corrode or be incompletely mated, solder joints fatigue under daily thermal cycling, and cables can be mechanically damaged. The consequences are:
- Ohmic losses: the power dissipated in a resistive fault scales with the square of the current (P = I²R).
- Local heating: a high resistance contact can reach temperatures that damage the connector and, in severe cases, create a fire risk.
- Limited detectability: a loss of a few percent in string output is difficult to distinguish from variations caused by irradiance, temperature and soiling in standard production monitoring.
As a result, such faults are often detected late, and localising them usually requires manual inspection of the plant string by string.
Measuring series resistance by impedance spectroscopy
emazys develops test equipment based on patented impedance methods. The handheld Z300 PVT instrument injects a small AC signal into a PV string and measures the voltage and current response over a range of frequencies. The complex impedance, Z = V/I, is obtained at each frequency.
The dynamic behaviour of a PV cell can be described by the series resistance Rs in series with the dynamic resistance of the diode rD, the shunt resistance Rsh, the depletion capacitance Cdep and the diffusion capacitance Cdiff [1, 3]. Combining the parallel elements into Rp = rD || Rsh and Cp = Cdep + Cdiff gives the simplified equivalent circuit:
Z(ω) = Rs + Rp / (1 + jωRpCp) (3)
In the complex plane, (3) describes a semicircle displaced from the origin by Rs. At low frequency the capacitive branch acts as an open circuit and Z → Rs + Rp. At high frequency it acts as a short circuit and Z → Rs. The two regions are separated by a single time constant τ = RpCp, with the maximum of the imaginary part at ω = 1/(RpCp) [1]. Since a module consists of series connected cells, the same model applies at module and string level with scaled parameter values [1, 4].
Two properties make this model suitable for field measurements. First, Rp depends strongly on the operating point: under illumination the diode is forward biased, rD becomes small, and the impedance approaches Rs over a wide frequency range [5]. Second, Rs itself is largely independent of the bias voltage, apart from temperature effects caused by Joule heating [1]. In practice Rs is extracted by fitting the measured spectrum to the equivalent circuit in the range from about 100 Hz to 10 kHz, above which the inductance of the DC cables causes the impedance to rise [5]. This avoids the conventional method of estimating Rs from the slope of the IV curve at open circuit voltage, which requires conditions close to STC. The same measurement principle is used in the Z300 PVT to locate insulation faults and interruptions along the string.
emazys instruments have recorded more than 227,000 string measurements on over 3,500 PV sites, covering more than 6.4 million PV modules. In approximately 11% of these measurements the series resistance exceeded 750 Ω, a value far above that of a healthy string and indicative of a severely degraded or interrupted conductive path. This share should not be interpreted as the fault rate of the general PV population. The dataset is biased towards faulty strings, since the Z300 PVT instrument is typically used for troubleshooting at sites where a fault is already suspected. With this limitation in mind, the dataset provides an empirical basis for defining reference values and fault thresholds.
From periodic inspection to continuous monitoring
A handheld instrument is typically used once a fault is already suspected, which makes the maintenance process reactive. SOLARIS aims to support predictive operation and maintenance of PV plants, with targets of a 40% reduction in the number of field investigations and a 50% increase in the number of investigations in which the root cause is identified. Meeting these targets requires measurements that are performed automatically and repeatedly, independent of site visits.
Within SOLARIS, emazys has therefore adapted the measurement technology of the Z300 PVT to a permanently installed monitoring PCBA and device. The first version implements the basic concept, and its main characteristics are:
- String connection: in the current version, the device is connected to the string with standard MC4 connectors, and the string is disconnected from the inverter while the device is connected. The existing installation is otherwise not modified.
- Automated measurement: impedance measurements are performed without an operator at regular intervals.
- Data integration: series resistance values are transmitted with a timestamp to the SOLARIS IoT platform developed by Elliot Cloud, where they are available to the other diagnostic and predictive maintenance tools of the project.
- Outdoor enclosure: the electronics are housed in a sealed enclosure for permanent outdoor installation.
Figure 1. Monitoring device developed by emazys in SOLARIS. Measurement electronics in a sealed enclosure with MC4 connections to the PV string.
Repeated measurements allow the evolution of series resistance to be followed over time for each string. A gradual increase can then be detected at an early stage, before it results in component failure or a measurable reduction in energy yield, and maintenance can be directed to the affected string.
First field installation
As a first step towards the demonstration phase, the monitoring device has been installed on a residential PV system in Denmark. The purpose of this installation is to operate the device on a real PV string under outdoor conditions before installation at the DTU demonstration site. The device is connected to a string of six LONGi LR5-54HIH-405M modules next to the inverter (Figure 2). In this first version, the string is disconnected from the inverter and connected to the device only.
Figure 2. Monitoring device (yellow enclosure, opened) installed on a six module string next to the inverter of a residential PV system.
The module datasheet values relevant for the evaluation are listed in Table 1.
|
Parameter (per module, STC) |
Value |
|
Module |
LONGi LR5-54HIH-405M |
|
Maximum power, Pmax |
405 W |
|
Open circuit voltage, Voc |
37.0 V |
|
Short circuit current, Isc0 |
13.83 A |
|
Voltage at Pmax, Vmpp |
31.0 V |
|
Current at Pmax, Impp |
13.07 A |
|
Modules in string |
6 |
Table 1. Module data for the test string.
Seven measurements were recorded on 9 October 2026. The first three measurements, taken between 08:40 and 09:16 during installation, show a string voltage close to 0 V and an impedance of approximately 400 kΩ, consistent with an open circuit before the string was connected. The four subsequent measurements on the connected string are listed in Table 2.
|
Time |
Voc (V) |
Riso (MΩ) |
Rs (Ω) |
Status |
|
09:21:24 |
208.2 |
114.6 |
5.6 |
OK |
|
09:23:40 |
208.0 |
229.8 |
7.8 |
OK |
|
09:24:02 |
208.1 |
23.3 |
7.7 |
OK |
|
09:25:24 |
208.2 |
10.3 |
7.8 |
OK |
Table 2. Measurements on the connected six-module string, 9 October 2026.
The measured series resistance was between 5.6 Ω and 7.8 Ω (mean 7.2 Ω), and the isolation resistance was above 10 MΩ in all measurements, well above the 1 MΩ level used as a fault threshold.
To evaluate whether the series resistance is within the expected range, the measured value is compared with a worst-case limit derived by emazys from a study of more than 500 commercial PV modules of different technologies and sizes [5]:
Rs,max = 30 Ω·A × (Voc / 100 V) × (1000 W/m² / G) / Isc0 (4)
where Voc is the open-circuit voltage of the string, G is the in-plane irradiance, and Isc0 is the module short-circuit current at STC. With Voc = 208.2 V and Isc0 = 13.83 A, the limit becomes Rs,max = 4.5 Ω × (1000 W/m² / G). Table 3 lists the resulting limit for a range of irradiance levels.
|
Irradiance G (W/m²) |
Rs,max (Ω) |
|
100 |
45.2 |
|
200 |
22.6 |
|
300 |
15.1 |
|
400 |
11.3 |
|
500 |
9.0 |
|
600 |
7.5 |
|
800 |
5.6 |
|
1000 |
4.5 |
Table 3. Maximum allowed series resistance for the test string as a function of irradiance.
The highest measured value, 7.8 Ω, is below the limit for irradiance levels up to approximately 580 W/m². Irradiance was not recorded during this test. For a morning measurement in October at Danish latitude, the in-plane irradiance is expected to be below this level, and the string is classified as healthy, in agreement with the status reported by the device. The limit decreases at high irradiance, which shows that series resistance values should be interpreted together with the irradiance at the time of measurement. Irradiance data will therefore be included in the evaluation during the demonstration phase.
Next steps
The device will remain in operation to collect a time series of series resistance under varying conditions, which will be used to assess measurement repeatability and the influence of irradiance and temperature. The next development step is a version of the device that operates in-line, so that measurements can be performed while the string remains connected to the inverter and in production. In parallel, laboratory testing continues under conditions defined together with DTU. The device will subsequently be installed at the DTU demonstration site and evaluated together with the other SOLARIS tools at the project demonstration sites, with the aim of establishing criteria for early fault detection based on series resistance trends.
References
[1] M.-I. Oprea, Fault detection in PV arrays using advanced characterization methods, MSc thesis, Aalborg University, 2015 (supervisors D. Sera, A. R. Andersen, R. Basu).
[2] S. M. Sze and K. K. Ng, Physics of Semiconductor Devices, 3rd ed., Wiley, 2006.
[3] I. Mora-Seró, G. Garcia-Belmonte, P. P. Boix, M. A. Vázquez and J. Bisquert, Impedance spectroscopy characterisation of highly efficient silicon solar cells under different light illumination intensities, Energy Environ. Sci. 2, 678, 2009.
[4] R. L. Mueller, M. T. Wallace and P. Iles, Scaling nominal solar cell impedances for array design, Proc. IEEE 1st WCPEC, vol. 2, pp. 2034-2037, 1994.
[5] emazys, String Test Application Note, emazys ApS, Odense.